Overview
A scratch is a single line of damage from one hard point: grit under a boot, the corner of a pallet, a dropped tool dragged aside. The sclerometer test measures the force it takes to make one.
What the test measures
The test measures the load at which a hard, rounded tip leaves a mark in the cured film. The result is given in newtons, written N.
How the test is carried out
A sclerometer is a hand-held instrument shaped like a pen. Inside is a spring that presses a tungsten carbide tip against the surface. A slider sets the spring force, which is read off a scale on the barrel.
- The coating is applied to a rigid panel and left to cure fully.
- The spring is set to a low force and the tip is drawn across the film in a short line.
- The force is raised in steps, with a fresh line each time.
- The result is the force at which the tip first leaves a visible scratch.
ISO 1518 describes the laboratory version of the same idea, in which a loaded stylus is drawn across the panel by a machine.
How to read the result
Higher is better. A coating marked at 10 N resists scratching more than one marked at 4 N, on the same instrument and tip.
The result should say what counted as failure. A first visible mark and a scratch through to the substrate are different points, and the second needs far more force.
What it means in use
Scratch resistance is about single events, not steady wear. It shows how a floor copes with grit and dragged edges, and how a painted gate or machine copes with knocks from tools and keys.
What the result does not tell you
The instrument is hand-held, so the result depends on the operator: the angle, the speed and what they judge to be a visible mark. It is best used to compare coatings tested by the same person on the same day.
Results from different instruments or tip sizes cannot be compared. A smaller tip concentrates the same force on a smaller area.
A thin film on a soft substrate scratches more easily than the same coating applied thicker on a hard one. The figure belongs to the system tested.
Scratch resistance is not wear resistance. For steady rubbing wear see Abrasion Resistance (Taber Abrasion).
On our product pages
Where a product has been tested, its page shows the result, the method and, where the method has one, the rating. Results published on this site come from internal testing to the stated method. They are given for technical reference and comparison.
If a figure you need is not shown, ask our technical team.